Text from the interactive explanation
Design, Synthesis, and Characterization of a Novel Tetra-Block Copolymer for High-Performance Self-Healing Batteries
Avcı Yayla Iİ, Taskin OS, Yuca N.
Polymers 2025 · a self-healing binder for silicon anodes
Silicon could let a battery's anode store about ten times more charge per gram than the graphite used today. The catch: every time it charges, silicon swells to roughly four times its size — and the electrode slowly tears itself apart. Researchers in Istanbul designed a polymer “glue” whose broken strands can find each other again. Could that keep a breathing silicon electrode in one piece?
Silicon particle
Lithium ion
Copper foil (collects the current)
Carbon additives
Stranded particle — no electrical path
Teaching model · an illustrative simulation of the mechanism, not the paper's data. *Share of silicon with an electrical path to the copper at the end of the last cycle. The measured results come later.
Try it: drag the charge level to swell the particles yourself, or step one cycle at a time. Which electrode keeps more of its silicon connected to the copper — and why do grey particles stop glowing?
1 · Why silicon?
Ten times the room, four times the size
A lithium-ion battery charges by pushing lithium into its anode , the negative electrode. How much charge each gram of anode can take in and give back is measured in mAh/g (milliamp-hours per gram).
Graphite anodes manage about 372 mAh/g in practice. Silicon's theoretical capacity is about 3,500 mAh/g , because a single silicon atom can host up to 4.4 lithium atoms. Silicon is also abundant, cheap and non-toxic.
Before you fill it: when silicon is completely full of lithium, how big do you think it gets?
Make a guess, then drag the slider.
Graphite 0 of ~372 mAh/g
Silicon 0 mAh/g · 1.0× volume
2 · Why it breaks
One breath is fine. Hundreds are not.
Cycle 0 — a fresh particle, fully connected.
Each silicon particle in the paper's electrodes is only 30–50 nanometres across, far smaller than a bacterium. Every charge, it swells; every discharge, it shrinks. Repeat that hundreds of times and a chain of damage unfolds:
Swell. Lithium floods in; the particle grows by more than 300 %.
Stress. Neighbours push back and the binder holding everything is stretched.
Crack & disconnect. Particles fracture (“pulverization”) and binder links snap, so pieces lose their electrical path to the copper.
Crust regrows. Fresh surfaces react with the electrolyte and grow more SEI.
Capacity fades. Stranded silicon and lithium locked in the crust no longer store charge.
SEI, the solid–electrolyte interphase, is a thin crust that forms where the liquid electrolyte breaks down on the anode surface. A stable SEI protects the electrode — but building it uses up lithium, and every crack exposes new surface for more crust.
Try switching the binder, then scrub the cycles again. What still accumulates, and what is rescued?
3 · The binder
The glue's quiet job
An anode is not a solid slab of silicon. It is a paste of ingredients, spread onto copper foil with a blade and dried. In this study the recipe was:
Common binders such as PVDF and CMC/SBR mostly act as a mechanical scaffold. In the authors' words, PVDF is “largely inert”, and CMC/SBR offers “fewer active binding sites”. When the silicon swells and a link tears, it stays torn.
Self-healing polymers are materials that repair damage on their own. Some carry tiny capsules of healing agent; others, like the one in this paper, rely on reversible attractions between chains that can let go and grab on again. The question became: what if the glue's broken ends could find their partners again?
4 · The healing polymer
Four building blocks, two reversible grips
The new binder, PHX-23 , is a tetra-block copolymer: one long chain built from four different small molecules (monomers). Tap a building block to see what it brings.
How it is made: the four monomers are dissolved in chlorobenzene, an initiator (dibenzoyl peroxide) creates a reactive “radical” chain end, and the chain grows monomer by monomer — free-radical polymerization. PHX-23 was made at 80 °C for 48 hours under nitrogen, then precipitated and dried into a powder.
Scheme 1, “Synthesis of PHX via free-radical polymerization”, from Avcı Yayla, Taskin & Yuca, Polymers 2025, CC BY 4.0. Reproduced unmodified.
The cut-and-heal lab
The authors credit healing to two non-covalent (reversible) attractions working together: oily C18 tails that cluster together (hydrophobic association) and –OH groups that form hydrogen bonds . Cut the film, press it back together, then pull.
Intact film · 100 % of links in place
5 · Finding the recipe
Twenty-four tries to find one
Getting a glue that heals and works inside a battery took 24 recipes. The polymer had to come out as a clean powder, disperse in the coating solvent (NMP), survive the electrolyte without dissolving, and let the electrolyte wet the electrode. Tap any vial to open its lab-notebook entry.
PHX-23
Recipes from Table S1 (molar concentrations, temperature, time) and outcomes from the Results section of the paper. Table S1 labels the acid column “MMA”; the text names the monomer methacrylic acid (MA).
6 · What was measured
Into the coin cell
To test the binder, the team built silicon electrodes with PHX-23 and sealed them into coin-sized test cells (CR2032) facing a lithium-metal disc. This kind of cell is called a half-cell. Then they charged and discharged them again and again. Speed is given as a C-rate : 1C means a full charge in about an hour; C/5 means about five hours.
A thousand charges
Before you scrub: at cycle 500, which electrode do you think stores more?
Read the comparison carefully: the CMC-SBR cell ran at the gentler C/5 for 500 cycles (502 mAh/g at the end); the PHX-23 cell ran five times faster, at 1C, for twice as many cycles. Around cycle 500 both sit near 500 mAh/g. The authors conclude that PHX-23 shows superior cycle performance to CMC-SBR.
The speed dial
Pick a charging speed. The cell was run five cycles at each rate, from slow to fast, then back down.
Choose a speed.
Why faster means less: the cell's internal resistance under current creates an extra voltage loss (overpotential). The cell reaches its voltage limit sooner, so less capacity is delivered. When the rate came back down, the electrode “kept operating normally”.
Look inside the electrode
The authors report no cracks on the PHX-23 electrode after cyclic voltammetry (CV, a slow sweep of the voltage up and down). They also saw the silicon particles change from crystalline to amorphous (disordered), as expected after lithium has moved in and out. Panels cropped from Figure 6, Avcı Yayla et al. 2025, CC BY 4.0.
Impedance measurements (EIS) showed the resistance to moving charge across the electrode surface fell by 86 % after cycling. The authors attribute this to the binder repairing microcracks and keeping conductive pathways between silicon and carbon. Silicon's own swelling also improves contact.
In cyclic voltammetry, the currents became repeatable and the SEI layer stabilised from the fourth cycle. The authors link this to PHX-23's many functional groups anchoring to the silicon surface.
Thermal analysis: PHX-23 starts degrading at about 250 °C (glass transition 112 °C). That is well above typical electrode drying temperatures of 80–120 °C.
Electron microscopy of the polymer itself showed a highly porous, interconnected structure. Such porosity can buffer silicon's volume changes. EDX maps showed carbon, oxygen and nitrogen spread evenly.
NMR gave a molecular weight of about 2,480 g/mol, which is low for a polymer. It helps processing but limits thermal stability. The authors suggest exploring longer, higher-molecular-weight versions.
7 · Back to the question
What this brings closer
Can a glue that heals itself keep a breathing silicon electrode in one piece? In this lab test, it helped a lot. The electrode still faded, from 2,885 to 427 mAh/g. But after 1,000 fast cycles it kept a useful capacity above that of graphite anodes , and the electrode showed no cracks after cycling.
The authors are careful about what this means. It is not an immediate replacement for graphite . It is evidence that a self-healing binder can slow the damage and extend the practical use of silicon anodes toward real-world applications. PHX-23 is a proof of concept , so far made only at laboratory scale and tested in half-cells. Its ingredients are commercially available, and its simple free-radical synthesis is in principle compatible with large-scale processing. It is not yet economically competitive with established binders such as PVDF or CMC.
Next steps, in the authors' words: reaction optimisation, cost-efficient and environmentally benign synthesis, and longer-chain (higher molecular weight) versions that may be more flexible.
Scroll back to the top and watch the two electrodes again. You now know why the grey particles go dark — and what the teal strands are doing when they flash.
Source & credits
Işık İpek Avcı Yayla, Omer Suat Taskin and Neslihan Yuca. “Design, Synthesis, and Characterization of a Novel Tetra-Block Copolymer for High-Performance Self-Healing Batteries.” Polymers 17(17), 2414 (2025). doi:10.3390/polym17172414
Affiliations: Enwair Energy Technologies Corporation, Istanbul; Department of Chemical Oceanography, Institute of Marine Science and Management, Istanbul University; Energy Institute, Istanbul Technical University. The project received funding from the European Union's Horizon Europe research and innovation programme under grant agreement 101103702 (PHOENIX).
The article is open access under the Creative Commons Attribution 4.0 (CC BY 4.0) licence. Reused here: Scheme 1, Figure 3 and Figure 5 (unmodified); Figure 6 (cropped into before/after panels); Figure S1 (cropped from the Supplementary Materials); Video S1 (cropped, re-encoded, sound removed). The cycling and rate charts are re-plotted from values traced off Figures 5a, 5b and S1, so they are approximate. Numbers quoted in the text come from the paper.
All simulations on this page (the breathing electrodes, the single particle, the polymer chain and the cut-and-heal lab) are illustrative teaching models of mechanisms described in the paper. They are not reproductions of its data.
Topics in this iPaper
Chemistry
Monomers with functional groups were polymerized using the free radical polymerization method.
Section 2.1, Synthesis of Tetra-Block Copolymer; Section 3, Results
Engineering
The electrodes were used to assemble the coin cells (CR2032) while Li metal was used as a counter electrode.
Section 2.2, Electrode Preparation and Battery Assembling
lithium ion batteries
These results position PHX-23 as a transformative binder for silicon anodes in next-generation lithium-ion batteries.
Abstract
silicon anodes
a novel self-healing copolymer (PHX-23) was synthesized for Si anodes
Abstract
self healing polymers
The self-healing capability of the copolymer can be ascribed to the synergistic contribution of two non-covalent interactions
Section 3, Results
polymer binders
advanced polymer binders serve as essential components for preserving the structural integrity of Si-based anodes
Abstract
free radical polymerization
Synthesis of PHX via free-radical polymerization.
Section 3, Results (Scheme 1)
electrochemical impedance spectroscopy
EIS measurements were performed both before and after the CV with the aim to better understand how the polymer affected Si anodes.
Section 3, Results (Figure 4b)