An Elastocaloric Polymer with Ultra-High Solid-State Cooling via Defect Engineering

Zhaohan Yu, Duo Xu, Zumrat Usmanova, Chuwei Ye, Aditya Swarnkar, Emma Scott, Sizhe Huang, Siyuan Rao, Xinyue Liu, Svetlana V. Boriskina, Ruobing Bai, Shaoting Lin

Pull a rubbery ribbon fast and it warms. Let it snap back and it cools — no refrigerant gas involved. Could solids like this one day help cool hot electronics, factory equipment, or people working in extreme heat? This study found that the polymer cools best when its molecular net is a little bit broken.

Heat hidden in a stretch

A polymer is a material built from very long chain molecules. In a rubbery polymer the chains are tied together into a loose net. At rest, each chain is coiled up like cooked spaghetti, constantly wriggling with heat.

Pull, and the chains uncoil and line up along the pull. Once they are lined up well enough, neighbouring stretches of chain can snap into tiny, orderly bundles — crystals. This is called strain-induced crystallization , or SIC.

Snapping into a crystal gives off energy as heat, called latent heat — the same kind of heat water gives off as it freezes. Melting the crystals soaks that heat back up.

If the pull is fast, the heat has no time to escape, so the material itself gets hotter. A change that fast is called adiabatic. Warming on a fast stretch and cooling on a fast release is the elastocaloric effect .

Try it: drag the slider or drag across the picture.

A stretched ribbon has cooled back to the room's temperature. You let go. What happens?

Pick an answer to reveal the full cycle.

Natural rubber, the classic stretchy material, crystallizes only about 15% when pulled to six times its length, giving a swing of about 3.5 °C at around 55 °C. More crystal per stretch should mean a bigger swing — so the question is how to get more.

The paper quotes a standard thermodynamic estimate of the adiabatic temperature change:

The first term is the crystal heat; the second is the heat from simply straightening chains. The authors point out that measured swings stay well below this estimate, and that such models usually ignore topological defects — flaws in how the net is connected, which almost every real polymer has. That gap is what this study probes.

A nearly perfect net — broken on purpose

The material here is an end-linked star polymer (ELSP) . Its building blocks are star-shaped molecules of PEG (polyethylene glycol) with four arms each. One kind of star has amine groups at its arm tips; the other has NHS groups. An amine tip and an NHS tip click together, so the two kinds link arm-to-arm into an unusually regular net: every chain has the same length and there are almost no tangles.

The net is made in water as a gel, then dried into a solvent-free rubbery solid that melts at about 45 °C . Below that it is partly crystalline and stiff; above it, it is rubbery and crystallizes mainly when stretched.

To add flaws on purpose, the team let the NHS stars sit in water before mixing. There, NHS tips slowly “go dead” (they hydrolyze) and can no longer link. The longer the wait, the fewer links form:

Reaction efficiency p — the fraction of arm tips that actually link. Defect density P — the chance that a given arm ends up a dangling chain: a loose end that carries no load.

P was worked out from how stiff each gel was, using a model of nets with defects, and checked with a fluorescent dye (fluorescamine) that lights up unlinked amine tips. With more defects, the same 60 g weight stretches a strip further (Fig. 1E): the net gets softer.

Stars with dangling arms — 1st order: 0 · 2nd: 0 · 3rd: 0 · 4th: 0

Two tugs in opposite directions

So what do loose ends do to crystals? Measuring crystallinity with X-rays and with heat-flow scans (DSC), the paper finds two effects pulling opposite ways. Choose a defect level to compare.

Stretched while hot

λ = 11 at 60 °C, above the melting point · X-ray crystallinity

Defects suppress stretch crystals: loose ends get in the way of chains lining up and of crystals orienting together.

Cooled without stretching

λ = 1, crystallizing on cooling · DSC crystallinity

Defects promote crystals that form on cooling (temperature-induced crystallization, TIC): a more flexible net crystallizes more readily.

Stretched below the melting point (λ = 11 at 40 °C), both kinds of crystal coexist and the total stays nearly the same, about 50% for every defect level (Fig. 2I) — the two effects balance. ≈ Read from Fig. 2I

Your prediction

In the hot chamber (above the melting point), which defect level will cool the most when released? You will test it in the lab next.

No prediction yet.

A clue from tearing tests

Below the melting point (25 °C), the energy needed to tear the material rises and then falls with defects:

16.50 → 20.16 → 15.78 kJ/m²

lowest defects → P = 0.22 (peak) → highest defects. Non-monotonic trends like this hint that the balance between flexibility and alignment matters. Measured · Fig. 3G

Pull, hold, release

This is the paper's key experiment. Pick one of the four ribbons the team tested, stretch it to 11 times its length in a hot chamber, hold it, then let it snap back. Watch the surface temperature, and fill your notebook to find which ribbon cools the most.

Nothing tested yet. Each completed release adds that ribbon's average jumps here.

Cooling on release, Fig. 4D Measured

The chamber sits above the polymer's ≈45 °C melting point, so the ribbon stays rubbery. Why the slow creep after each jump? Stretched, the ribbon reaches into the hotter chamber centre (≈85 °C) and keeps warming a little; released, it sits back near the ≈65 °C end and re-equilibrates. A control with non-stretchy PLA plastic showed only this slow drift and no jumps, so the sudden jumps come from the polymer itself (Supporting Information, Fig. S12).

The authors' interpretation

The authors attribute the peak to the two tugs from Chapter 3. With few defects , chains align strongly but the net is stiffer and less flexible. With moderate defects , chains still align well, and the extra flexibility helps them crystallize. With many defects , too many loose ends disrupt alignment and stretch crystallization drops.

A simple “mean-field” model in the paper (one that treats defects as spread evenly) reproduces this competition qualitatively.

Reading the evidence

Here are the paper's averages for all four ribbons. Each bar is the mean of repeated measurements; the error bar on the best ribbon is one standard deviation, and the dots show its individual releases.

Peak at P = 0.22: +31% vs P = 0.09 (stated).

Peak at P = 0.22: +39% vs P = 0.09 (stated). Individual releases ≈9.2, 9.1 and 6.1 °C — the 6.1 °C one is the representative trace you can overlay in the lab.

As compiled by the authors (Table S3; one more liquid-crystal elastomer at ≈125 °C, ≈1 °C, is off this axis). Ambient temperatures for this study are plotted at 65–70 °C, i.e. “above 65 °C”.

In hot conditions, this ELSP leads the authors' comparison: 8.14 °C versus 1.8 °C for natural rubber tested the same way (about 350% higher).

Near room temperature, several materials swing more — SEBS (a block-copolymer rubber) 15.3 °C, latex rubber 14 °C — and the authors' earlier, nearly defect-free ELSP reached ≈9.3 °C at 55 °C. So the advance is about hot environments and about defects as a tuning knob , not an all-round record.

A separate test: does it keep working?

A useful cooling material must survive many stretches. The team ran 100 stretch–release cycles and compared each cycle's temperature jump with the first one.

Over 100 cycles the normalized jumps stay roughly between 0.82× and 1.24× of the first cycle — “relatively stable”, in the authors' words. This was measured on low-defect samples, so it does not by itself show how the best (P = 0.22) ribbon ages.

Back to the hot room

We started with a ribbon that cools when it lets go. The surprise of this study is which ribbon cools best: not the most perfect net, but one with a moderate share of loose ends. Defects, usually treated as flaws, become a design knob.

What changed

The best ribbon cooled about 39% more than the nearly perfect one and about 4.5 times as much as natural rubber in the same hot setting. Measured ≈ 5.9 read from Fig. 4G

What it could enable — the authors' hopes

Because it works best when hot, the authors suggest defect-engineered ELSPs as candidates for high-temperature uses: managing waste heat, cooling hot spots in high-power electronic and industrial equipment, and wearable cooling for people exposed to extreme heat. They also mention heat-driven actuators and energy harvesting. These are possibilities, not demonstrations.

What it is not (yet)

Single jumps, small samples Temperature jumps of small specimens during single fast stretches and releases in a lab chamber.

Hot-only Tested with the ambient above 65 °C, above the ≈45 °C melting point. Near room temperature other polymers swing more.

A big stretch The ribbon is pulled to 11 times its length.

Four samples “Best near P = 0.22” means best of 0.09, 0.22, 0.34 and 0.47.

Spread 8.14 ± 1.76 °C on average; the representative single release was 6.1 °C.

Room to grow Measured swings are still far below the thermodynamic estimate, and the model assumes evenly spread defects.

Next steps the authors name: measuring cooling over repeated, non-equilibrium cycles; thermal conductivity; molecular simulations; how the speed of stretching matters; and a different defect type — closed loops in the net — which they expect could help even more but have not tested.

Source & credits

Zhaohan Yu, Duo Xu, Zumrat Usmanova, Chuwei Ye, Aditya Swarnkar, Emma Scott, Sizhe Huang, Siyuan Rao, Xinyue Liu, Svetlana V. Boriskina, Ruobing Bai, Shaoting Lin. “An Elastocaloric Polymer with Ultra-High Solid-State Cooling via Defect Engineering.” Advanced Science 13, e18106 (2026). Published online December 12, 2025.

DOI: 10.1002/advs.202518106 · open-access PDF · Open access under the Creative Commons Attribution License (CC BY 4.0).

All visuals are original code drawings; charts redraw data read from Figs. 1D, 2C, 2F, 2I, 3G, 4B–4H, S16 and Table S3 of the paper and its Supporting Information (values marked ≈ are approximate). The test conditions come from the paper's Supporting Information. Interpretation of mechanisms follows the authors. Lab trace shapes are illustrative model curves; their jump heights are the paper's averages.

Fonts: Fraunces, Inter and IBM Plex Mono (SIL Open Font License).

Topics in this iPaper

Engineering
waste-heat management and localized cooling in high-power electronic and industrial equipment

Discussion, page 8

Chemistry
tetra-NHS-terminated PEG macromers (PEG-NHS), cross-linked via amine-NHS bonds

Section 2.1, page 2

Physics
develop a thermodynamic model to systematically analyze the impact of dangling-chain defects on crystallization

Introduction, page 2

elastocaloric effect
SIC further uniquely enables an emerging cooling technology known as solid-state elastocaloric cooling

Introduction, page 2

strain induced crystallization
Strain-induced crystallization (SIC) is a ubiquitous phenomenon commonly observed in polymeric materials

Introduction, page 1

topological defects
the role of topological defects remains unexplored despite their prevalence in real polymers

Abstract, page 1

polyethylene glycol
tetra-arm poly(ethylene glycol), topological defects

Keywords, page 9

solid state cooling
elastocaloric polymers, solid-state cooling, strain-induced crystallization

Keywords, page 9